Test method for coating amount of PTP aluminum foil protective agent

Test method for coating amount of PTP aluminum foil protective agent

2022-12-12

Test method for coating amount of PTP aluminum foil protective agent

The protective agent layer of PTP aluminum foil is a dense cross-linked resin layer formed by high temperature curing. It is difficult to completely wipe the coating in a short time by the solvent wiping method commonly used now, and it is difficult to obtain accurate coating quantity value. Moreover, the repeatability of sample test results is also very poor. Therefore, a more effective test method for the coating quantity of PTP aluminum foil protective layer is found, It is of great practical value to guide the production of such products.

According to the material characteristics of PTP aluminum foil and the comparison of the advantages and disadvantages of various detection methods, we finally believe that the "burning method" is the most suitable for the rapid detection of the amount of protective agent coating:

In this method, the PTP aluminum foil sample is placed in a muffle furnace, maintained at a certain temperature for a certain time, and the PTP aluminum foil coated with the protective agent layer is baked at high temperature, so that the protective agent layer is completely oxidized and gasified. The coating amount of the protective agent layer can be calculated by detecting the quality of the aluminum foil before and after the high-temperature baking.

1、 Instruments and reagents:

10cm * 10cm standard cutting plate, blade, analytical balance (precision: 1/10000 g), muffle furnace, glass plate, stainless steel tweezers, ethyl acetate (analytical pure), absorbent cotton

2、 Test method:

1. Select the aluminum foil sample sheet for drug packaging with flat surface and no wrinkles, cut 5 test samples with a blade and a 10cm * 10cm standard cutting plate, and control the deviation of the width and length of the sample within ± 0.5mm

2. Weigh the cut sample (W1) on the balance.

3. Put the printing face of the aluminum foil on a glass plate, and use stainless steel tweezers to clamp the degreased cotton dipped in ethyl acetate to wipe the heat-sealing coating surface of the aluminum foil until no obvious marks can be identified when the surface is observed with naked eyes. (Note: The cotton ball dipped with ethyl acetate shall not have the liquid of ethyl acetate dripping. The circular wiping method from the center to the edge shall be used for wiping. The edge of the aluminum foil must be laid flat on the glass plate, and the linear wiping method shall be used for wiping. The other side of the aluminum foil shall not be affected during the whole process as much as possible). If the cotton ball has been wiped with the printing coating, replace it with a new cotton ball.

4. After wiping the heat-sealing coating, put the aluminum foil in a ventilated place and place it at room temperature for 2 minutes.

5. Then weigh the weight (W2) on the analytical balance

6. Place the above aluminum foil on the sample shelf in the muffle furnace preheated to 550-600 ℃. After waiting for a period of time, take out the coated aluminum foil and place it at room temperature. (The black ink may not completely volatilize the pigment, and its impact can be temporarily ignored for the products with general printed text patterns. If the printed patterns are large, the weight impact of the ink binder and the pigment should be considered)

7. Then weigh the weight (W3) on the analytical balance

Note: If the test sample has no adhesive layer, omit the operations in 2, 3 and 4.

8. Result calculation:

(W1-W2) × 100=weight of heat seal layer (g/m2)

(W2-W3) × 100=weight of printing layer/protective layer (g/m2) (when the sample has adhesive layer)

(W1-W3) × 100=weight of printing layer/protective layer (g/m2) (when the sample has no adhesive layer)

W3 × 100=weight of aluminum foil layer (g/m2)

Calculate and report the test results and average values of all individual samples to the nearest 0.01g/m2.


主站蜘蛛池模板: 精品乱码一区内射人妻无码| 无码精品人妻 中文字幕| 国产精品无码成人午夜电影| 94久久国产乱子伦精品免费| 中文字幕日韩人妻在线视频| 国产精品久久久久蜜臀| 国产成人精品亚洲777人妖| 岛国av动作片在线观看| 无码ol丝袜高跟秘书在线观看| 天堂资源官网在线资源| 亚洲午夜精品一区二区| 夜夜爽夜夜叫夜夜高潮漏水| 狠狠噜天天噜日日噜av| 亚洲成在线aⅴ免费视频| 亚洲精品成人片在线观看精品字幕| 少妇脱了内裤让我添| 天堂а√中文最新版地址在线| 国产欧美一区二区精品性色| 国内精品自在自线| 娜娜麻豆国产电影| 少妇与子乱毛片| 亚洲产国偷v产偷v自拍色戒| 国产精品国产对白熟妇| 成人国产一区二区三区| 人人入人人爱| 国产日产欧产精品精品app| av午夜久久蜜桃传媒软件| 欧美无人区码suv| 精品人妻系列无码专区| 日本高清无卡码一区二区久久| 色翁荡熄又大又硬又粗又视频图片 | 亚洲成a v人片在线观看| 亚洲欧美国产双大乳头| 亚洲精品综合一区二区三区在线| 奇米影视第四色首页| 午夜男女很黄的视频| 用舌头去添高潮无码视频| 中文字幕av伊人av无码av| 久久aⅴ免费观看| 成人免费xxxxx在线观看| 久久午夜无码鲁丝片午夜精品|